Fix Your Bend: A Rotary Draw Troubleshooting Chart
The 12 most common shop-floor problems, with tooling-based solutions.
Use the filters to view defects by type: wrinkling, humps and collapse, or marks and scratches.
1Humps and collapse
Hump at end of bend
Solution
- Relocate mandrel back from tangent until bump is barely visible (this is a good system to find the best location for a mandrel.)
2Wrinkling
Wrinkling throughout bend and even extending into wiper die areas
Solution
- Advance wiper die closer to tangent.
- Decrease rake of wiper die.
- Wiper worn out – have replaced.
3Marks and scratches
Bad mark at start of bend and over bend for 90°
Solution
- Removable clamping portion of bend die not matched properly to round part of bend die.
- Clamping portion of bend die not parallel to the key way.
4Wrinkling
Wrinkling occurring for only a portion of the bend (45° out of 90°.)
Solution
- Bend die groove and counter bore are not concentric.
- Taper in pressure die (from bottom of tube groove to back of die.)
5Wrinkling
Wrinkling throughout bend area with wiper and mandrel in known proper position
Solution
- Check for undersized mandrel.
- Increase pressure die force only after checking wiper fit and mandrel location.
6Humps and collapse
Excessive collapse with or without wrinkling throughout entire bend
Solution
- Advance mandrel toward tangent until slight hump occurs (most mandrels must project somewhat past tangent.)
7Humps and collapse
Mandrel ball humps
Solution
- Too much drag on tube; back off pressure die force – increase wiper die rake.
- May require closer pitch mandrel ball assembly.
- Tubing material too soft.
8Humps and collapse
Excessive collapse after tubing is pulled off mandrel balls
Solution
- Check for too much drag on tube; back off pressure die force, increase rake in wiper die, etc.
- Increase mandrel support, change from a plug to a one ball, from a 2 ball to a 3 ball mandrel, etc.
9Wrinkling
Heavy wrinkle through bend area only and linear scratches in grip area indicating slippage in clamp section
Solution
- Reduce pressure die force.
- Check location (and lube) of mandrel and wiper die.
- Increase pressure on clamp die. Use serration, knurling or carbide spray in clamp area.
10Marks and scratches
Tool marks on center of bend
Solution
- Oversized tube.
- Re-adjust vertical alignment of clamp and/or pressure die.
- Undersized tube groove in bend die.
11Marks and scratches
Deep scratches throughout the bend and in wiper die area
Solution
- Increase rake or relief in wiper die 1 to 2 degrees.
- Use more and/or better lubrication.
- Galled tube groove in wiper die – Recut wiper die.
12Marks and scratches
Tool marks on center line of bend in clamp and pressure die area
Solution
- Reduce pressure die force.
- Oversized tube or undersized tube groove.
Before you bend
When it comes to making a perfect bend, several factors come into play:
- Determine that the bender you will be using is operating properly.
- Make sure the clamping and unclamping of dies, rotation of swing arm, and extracting of mandrel are all occurring in the proper sequence.
- Make sure the tube you will be using is clean, both inside and outside.
- Check the tooling, making sure it is clean, burr free, and compatible with the tube to be bent.
- Confirm that the mandrel is the required distance past the tangent.
Still stuck? Send us your tube size, bend radius and machine details, and we will help you find the cause.